Hướng dẫn về thử nghiệm trong phòng thí nghiệm và đánh giá hiệu suất của chất làm đặc trong in ấn

Laboratory evaluation of a printing thickener should cover more than one viscosity result. This guide...

Việc đánh giá trong phòng thí nghiệm đối với chất làm đặc dùng trong in ấn cần bao gồm nhiều kết quả đo độ nhớt khác nhau. Hướng dẫn này giải thích về quy trình kiểm tra bột, chuẩn bị hỗn hợp bột nhão, tính lưu biến, tính tương thích của công thức, các thử nghiệm in ấn, khả năng rửa trôi và đánh giá hiệu suất cuối cùng.

Printing thickeners control how a dye or pigment paste is prepared, transferred through the printing equipment, deposited on the fabric and removed or fixed during post-treatment. A product that develops high viscosity in water may still perform poorly after dyes, salts, alkalis, binders or other auxiliaries are added.

Laboratory testing should therefore follow the product through the complete application process. Dry-powder properties, hydration, rheology, formulation compatibility, print definition, color performance and wash-off should be evaluated as separate but connected stages.

The objective is not to identify the thickener with the highest viscosity. It is to identify the grade that provides suitable process behavior and repeatable printing results at an acceptable total cost in use.

What a Laboratory Evaluation Should Determine

A useful testing program should answer several practical questions:

  • Does the powder match the expected identity and physical condition?
  • Can it be dispersed and hydrated using the mill’s normal equipment?
  • How much product is required to reach the application viscosity?
  • Does the paste show suitable shear-thinning and recovery behavior?
  • Is viscosity stable after dyes and auxiliaries are added?
  • Does the paste pass through the screen and release evenly?
  • Does it control spreading and penetration on the selected fabric?
  • What are the effects on color yield, fixation, wash-off and fabric handle?
  • Can the supplier reproduce the approved performance in later batches?

These questions cannot be answered by one laboratory value. A complete evaluation normally moves from simple screening tests to controlled application trials.

Testing StageMain PurposeTypical Decision
1. Dry-powder evaluationCheck sample condition, consistency and handling propertiesAccept or reject for solution preparation
2. Stock-paste testingMeasure hydration, viscosity and rheological behaviorIdentify suitable dosage and preparation method
3. Complete-paste compatibilityEvaluate interaction with dyes, alkalis, salts, binders and auxiliariesConfirm formulation suitability
4. Controlled printing trialAssess screen behavior, transfer, penetration and definitionConfirm machine and fabric compatibility
5. Finished-print evaluationMeasure color, wash-off, fastness and handleConfirm final performance
6. Documentation reviewCompare results, specification, cost and batch-control supportApprove, adjust or reject the grade

Define the Printing System Before Testing

A thickener cannot be evaluated independently from its intended process. The laboratory should define the application before preparing the first sample.

Record the production requirements

  • Fiber and fabric construction
  • Reactive, disperse, pigment, vat, discharge or other printing route
  • Flat-screen, rotary-screen, roller or digital pretreatment process
  • Current paste formulation
  • Target application viscosity and test method
  • Screen mesh, engraving or application equipment
  • Drying and fixation procedure
  • Washing or reduction-clearing process
  • Yêu cầu về độ sắc nét in, độ thấm và cảm giác khi sờ vào vải

Select a reference product

Use the current production thickener or another approved grade as the reference. Testing a new product without a reference makes it difficult to decide whether the result represents an improvement or simply a different paste behavior.

The reference and candidate samples should be prepared and tested at the same time wherever possible.

Use two comparison approaches

First compare equal as-supplied mass where both products have comparable form and formulation. When comparing powder with liquid or formulated blends, record moisture, nonvolatile solids and verified active content separately; dry matter is not necessarily active thickener. State the chosen basis before interpreting efficiency or cost.

Then compare each product at the target application behavior under the same measurement and printing conditions. Matching one apparent-viscosity reading is a useful control, not proof of equal rheology. Record any dosage change and its effect on other formulation components.

Equal dosage helps screen thickening response on the stated product basis. A matched-viscosity trial helps compare printing under one controlled measurement condition. Neither comparison alone establishes equivalent complete-process performance.

Laboratory Equipment and Sample Controls

The exact equipment depends on the product and test program. A practical textile printing laboratory may use:

  • Calibrated laboratory balance
  • Controlled-speed mixer
  • Rotational viscometer or rheometer
  • Thermometer or controlled-temperature bath
  • pH meter
  • Moisture analyzer or approved oven method
  • Sieve set or particle-size equipment
  • Laboratory screen-printing equipment
  • Dryer and fixation equipment
  • Spectrophotometer
  • Microscope, scanner or controlled imaging system
  • Wash-fastness and rubbing-fastness equipment where required

Identify and condition samples

Record the supplier, product name, grade, batch number, receipt date, packaging condition and sampling source. Keep the original label or a traceable photograph with the test record.

Powder samples should be sealed and conditioned under the laboratory’s defined environment before testing. Moisture exposure during storage or sample preparation can affect powder weight and solution performance.

Stage 1: Dry Powder Evaluation

Dry-powder screening can identify obvious differences before time and dyes are used in printing trials.

Appearance and contamination

Check color, uniformity, visible foreign material, caking and unusual odor. Appearance should be compared with the supplier’s specification and the approved reference sample.

Appearance alone cannot confirm product identity or purity. A normal-looking sample may still differ in viscosity, moisture or chemical characteristics.

Độ ẩm

Water content, loss on drying and dry residue answer different analytical questions. An oven result can include water and other volatile losses under its stated conditions, rather than selectively measuring water. Dry residue can include salts and other nonvolatile ingredients; it is not automatically active polymer. State the method, denominator and any verified active-content assay before adjusting an as-supplied dose.

The test method, drying temperature, test time and calculation basis should be specified. Results from different moisture methods may not be directly comparable.

Particle size and powder handling

Particle-size distribution can influence dusting, wetting, lump formation and hydration time. Extremely fine powder may disperse differently from a coarser grade even when the final solution viscosity is similar.

Bulk density and flow behavior may also be recorded when they affect weighing, dosing, bag emptying or automated handling.

Product-specific chemical parameters

Depending on the chemistry and agreed specification, additional tests may include degree of substitution, active content, ash, insoluble matter or another identity-related parameter.

These tests should use a validated method appropriate to the individual product. Not every parameter is required for every printing thickener.

Stage 2: Standard Stock-Paste Testing

Write the preparation procedure for each comparison objective. A common incoming-QC method or existing factory SOP tests conformity or handling within that stated process. Separately, application qualification should prepare each grade by its documented route to a defined readiness endpoint. Record differences in addition order, activation, hydration and mixing; do not describe a grade that is unfinished at a fixed time as its fully prepared application performance. Nouryon’s CMC preparation guidance illustrates grade- and mixing-dependent dissolution; it does not prescribe one preparation time for other thickeners or an FSX grade.

Two people beside laboratory apparatus, with one person writing on a clipboard

Standardize the preparation procedure

Bản ghi:

  • Dry-product concentration
  • Whether concentration is calculated as supplied or on a dry basis
  • Water source and water quality
  • Water and powder temperature
  • Order and speed of powder addition
  • Mixer type, speed and mixing time
  • Resting or hydration time
  • Final sample weight and evaporation adjustment
  • Deaeration procedure

Powder should normally be added in a controlled manner to reduce lump formation. The appropriate addition method depends on product particle size, wetting behavior and supplier instructions.

Evaluate hydration behavior

Record the time required for the sample to become uniform and reach stable viscosity. Inspect for fisheyes, gel particles, undissolved powder, foam and sediment.

A product that reaches the target viscosity but requires impractical mixing time may create production problems during bulk preparation.

Measure viscosity under fully defined conditions

A viscosity result is incomplete unless it states:

  • Nồng độ sản phẩm
  • Sample temperature
  • Hydration or conditioning time
  • Mẫu máy đo độ nhớt hoặc máy đo lưu biến
  • Trục chính hoặc cấu trúc đo lường
  • Rotational speed or shear rate
  • Measurement duration
  • Đơn vị được báo cáo

Results measured at different concentrations, temperatures, spindle speeds or hydration times should not be compared as if they were equivalent.

Use more than one rotational speed

Printing pastes commonly show non-Newtonian behavior. Their apparent viscosity changes with the applied shear condition.

Measuring at multiple speeds provides information about shear-thinning behavior. A rheometer can provide a more complete flow curve and, where appropriate, information about yield behavior, thixotropy and viscoelastic response.

Evaluate recovery after shear

During screen printing, the paste is exposed to shear as it moves under the squeegee and through the screen. After deposition, it should recover enough structure to limit unwanted spreading.

A timed recovery test should specify preshear, high-shear exposure, rest or low-shear stage and measurement times. An increasing-and-decreasing speed sweep can show path dependence, but it is not automatically equivalent to recovery after screen transfer.

Measure pH and short-term stability

Measure pH at a defined concentration and temperature. After the established holding period, record viscosity drift, separation, skin formation and any unusual appearance or odor. These observations can trigger a contamination investigation but do not establish microbial growth or a microbial cause. Where that question affects release, use suitable sampling and a qualified microbiological method; no absence-of-odor check proves microbiological acceptability.

Stock-Paste TestWhat It IndicatesMain Limitation
Single-point viscosityApparent viscosity under one defined conditionDoes not fully describe shear-dependent behavior
Multi-speed viscosityRelative shear-thinning behaviorDepends on the instrument and measuring geometry
Flow curveViscosity or stress response across a shear rangeRequires a controlled rheological method
Recovery testHow structure rebuilds after shearMust reflect the intended printing process
Hydration observationMixing demand, lumping and solution uniformityCan be operator-dependent without clear criteria
pHGeneral solution condition and possible compatibility riskDoes not independently predict printing performance

Stage 3: Complete Printing-Paste Compatibility

Stock paste prepared only with water does not represent the complete printing formulation. Dyes, pigments, electrolytes, alkalis, binders, reducing agents and auxiliaries may change viscosity and stability.

Use the actual formulation

Prepare the complete paste using the same formulation and addition order used in production. Change only the thickener unless the trial is specifically designed to optimize the complete recipe.

If several dyes or pigments are used, test more than one representative color. Thickener interaction may be colorant-dependent.

Measure immediate and aged viscosity

Measure the complete paste after preparation and again after the normal production holding period. Record the storage temperature and whether the sample was remixed before testing.

A candidate that matches the initial viscosity but changes rapidly during storage may create shade or screen-performance variation during a production shift.

Check electrolyte and pH tolerance

Reactive printing pastes may contain alkali and other auxiliaries. Pigment systems may contain binders, catalysts and surfactants. Disperse or discharge printing introduces different compatibility requirements.

The test should reproduce the intended chemistry rather than using one universal salt- or alkali-tolerance procedure for every application.

Inspect filtration and screen residue

Where relevant, pass the paste through the production-equivalent filter or screen and inspect for gel particles, undissolved material and residue. Record the mesh or filter condition used.

Stage 4: Controlled Printing Trial

Laboratory printing should reproduce the intended process closely enough to reveal functional differences between samples.

Control the fabric

Use fabric from the same lot for all samples. Record fiber composition, construction, pretreatment, absorbency and conditioning.

Fabric-to-fabric variation can be larger than the difference between two thickeners, particularly when absorbency or pretreatment is inconsistent.

Control printing conditions

  • Screen mesh or engraving
  • Squeegee type, pressure, angle and speed
  • Number of printing strokes
  • Paste quantity or pickup
  • Printing direction
  • Time between printing and drying
  • Drying temperature and time
  • Steaming, curing or fixation conditions

Randomize or alternate the sample order where possible. Printing every candidate after the reference can introduce equipment, screen or drying drift into the comparison.

Use a diagnostic test pattern

The test design should include:

  • Fine positive lines
  • Fine reverse lines
  • Small dots
  • Diagonal and curved edges
  • Solid printed areas
  • Adjacent colors where bleeding is a concern
  • Light and dark shade areas

Record machine behavior

Observe screen passage, paste release, stringing, foaming, screen blocking, uneven transfer and drying on the screen. These observations should be recorded with defined rating criteria rather than general comments such as “good” or “poor.”

How to Measure Print Definition

Print definition should be evaluated using the same image-capture conditions for every sample. A calibrated scanner, microscope or fixed camera setup can be used.

Line-width change

Measure line width in declared fabric directions with the same image calibration and edge rule. Design or screen-opening width is a reference, not a unique spreading measurement: transfer, deposit, fabric deformation and later processing can also change final geometry. Where the cause matters, compare defined stages before and after drying/post-treatment and record relevant fabric dimensional change. Wider or broken lines guide investigation; they do not by themselves identify lateral flow or poor release.

Edge raggedness

Inspect whether the printed boundary is smooth or irregular. Edge irregularity may be related to paste rheology, fabric construction, screen condition or incomplete transfer.

Penetration and strike-through

Compare the face and back of the printed fabric. The required penetration depends on the textile product; maximum penetration is not always the objective.

A sharp face print with insufficient internal penetration may be unsuitable for some products, while excessive strike-through may reduce face color strength or pattern definition.

Stage 5: Finished Print Evaluation

Color yield and shade

Measure the printed fabric with a spectrophotometer using fixed instrument settings, sample conditioning, folding or backing and measurement geometry.

Relative color strength or K/S may be used when appropriate, but the measurement method and calculation should remain the same across all samples. Color yield should not be assessed visually alone.

Levelness

Measure several positions across the solid printed area. Report both the average result and variation between positions.

A high average color value may not be acceptable if the print is uneven or contains screen marks.

Rửa trôi

For dye-printing routes that require wash-off, use the same specified sequence for reference and candidate. Record temperature, liquor ratio, time, detergent and washing stages. For pigment printing, evaluate the cured binder system and required durability instead of treating removal of the film as the objective.

Assess residual thickener, unfixed color, staining, surface deposits and fabric handle. Wash-off should not be confused with wash fastness.

Tay cầm bằng vải

Handle can be assessed by a controlled panel or an appropriate instrumental method. Panel assessment should use coded samples and consistent conditioning to reduce bias.

Colorfastness

Select fastness tests according to the final textile and customer requirement. ISO 105-C06 provides methods for colorfastness to domestic and commercial laundering, while ISO 105-X12 addresses dry and wet rubbing.

A thickener should not be claimed to guarantee a specific fastness grade. Fastness also depends on dye or pigment selection, fixation, binder, washing and fabric.

Person handling a flask of purple liquid beside laboratory glassware

Product-Specific Testing Priorities

Thickener RouteTypical Evaluation FocusImportant Caution
Alginat natriReactive-dye compatibility, color yield, print definition, wash-off and viscosity stabilityCompare viscosity only under identical concentration and test conditions
Carboxymethyl celluloseDegree of substitution, hydration, rheology, dye interaction, wash-off and fabric handleCMC grades are not interchangeable by product name alone
FSX CMS commercial thickener gradesThickening efficiency, paste body, screen passage, penetration, wash-off and cost in useSuitability can vary between reactive, disperse, vat and compound systems
Compound ThickenerComplete-paste compatibility, storage stability, rheology and printing consistencyEvaluate the supplied formulation rather than only its main polymer
Digital Printing Pretreatment ThickenerFiltration, coating uniformity, fabric pickup, ink spreading, color and handleDo not apply screen-printing viscosity targets to digital pretreatment systems

How to Compare Samples Correctly

Use replicate preparations

When possible, prepare more than one independent paste from each sample. Repeating only the viscosity reading on the same cup does not measure variation in weighing, dispersion and hydration.

Thay đổi từng biến một

Keep the intended formulation, fabric, measurement conditions and printing/post-treatment route controlled. State whether a fixed-SOP handling challenge or grade-appropriate application preparation is being compared; record any necessary preparation differences. One-factor changes can test a local hypothesis but do not rule out interactions with the rest of the formulation.

If the complete formulation must be optimized, document each change and use an experimental plan rather than informal adjustments.

Use coded samples where possible

Coded samples reduce bias during visual assessment of powder appearance, print definition and fabric handle.

Report both performance and cost in use

Price per kilogram is not the same as application cost. Calculate the thickener dosage required to reach the target paste behavior and include preparation time, process stability and washing demand where reliable data are available.

Environmental or wastewater benefits should not be claimed unless they are supported by a defined test method and representative data.

Common Laboratory Testing Errors

Testing ErrorWhy It MisleadsBetter Practice
Comparing supplier viscosity values directlyConcentration, temperature, spindle and speed may differUse an agreed common QC/SOP test for its stated purpose; separately qualify application performance after each grade is properly prepared
Testing only at equal dosageMeasures thickening efficiency but not equal-viscosity performanceComplete both equal-dosage and equal-viscosity comparisons
Measuring immediately after mixingHydration may be incompleteDefine and verify the required hydration time
Ignoring sample temperatureViscosity is temperature-dependentCondition and record every sample temperature
Using different water sourcesHardness and dissolved salts may change hydrationUse one documented water source for comparisons
Testing only the stock pasteDyes and auxiliaries may change rheologyTest the complete printing formulation
Changing fabric lots between samplesAbsorbency variation can affect sharpness and colorUse one conditioned fabric lot
Reporting only the best printHides repeatability and levelness problemsReport replicate results and variation

Laboratory Report and Approval Decision

The final report should make it possible for another trained person to repeat the evaluation.

  • Supplier, product, grade and batch identification
  • Reference product information
  • Test objective and intended printing process
  • Dry-powder results
  • Stock-paste preparation procedure
  • Complete viscosity and rheology conditions
  • Complete printing-paste formulation
  • Fabric and printing conditions
  • Drying, fixation and washing procedure
  • Print definition and penetration results
  • Color, wash-off, fastness and handle results
  • Photographs or instrument files
  • Observed limitations and deviations
  • Technical and purchasing recommendation

Use a clear decision status

The conclusion may classify a sample as approved, conditionally approved, requiring reformulation, requiring production trial or rejected.

Conditional approval should identify the permitted application and any restrictions. A grade approved for disperse printing should not automatically be approved for reactive printing.

What Buyers Should Request from a Thickener Supplier

  • Bảng dữ liệu kỹ thuật
  • Bảng dữ liệu an toàn
  • Representative sample with batch identification
  • Viscosity specification with complete measurement conditions
  • Recommended concentration and preparation procedure
  • Relevant pH, moisture, DS or particle-size information
  • Recommended fabric and printing route
  • Compatibility and storage guidance
  • Batch COA for confirmed production where applicable
  • Grade-matching support based on the current product or TDS

Typical technical values should not be treated as guaranteed batch limits unless they are included in the agreed specification.

Sample and Grade-Matching Support from FSX Chemical

Two people reviewing an open catalogue beside a laptop, sample containers and documents

FSX Chemical supplies CMC, CMS, sodium alginate and digital printing paste for textile printing and related industrial applications. Sample selection should be based on the printing process and complete test conditions rather than on a general product name.

For a laboratory matching request, provide:

  • Current thickener name, TDS or physical sample
  • Fiber and fabric type
  • Hệ thống thuốc nhuộm, bột màu hoặc mực in
  • Printing and fixation method
  • Current formulation and thickener dosage
  • Target viscosity with concentration, temperature, spindle and speed
  • Main issue, such as unstable viscosity, spreading or difficult wash-off
  • Required packing and estimated purchasing quantity

FSX Chemical can review the supplied information and recommend a practical grade direction for sample testing. Final suitability should be confirmed through the customer’s controlled laboratory and production trials.

Ready to Test a Printing Thickener Sample?

Send FSX Chemical your current TDS, test method, paste formulation, fabric, dye system and target performance. Our team can help identify a suitable CMC, CMS, sodium alginate or printing paste route for comparison📧 Email: Service@fsxchemical.com

Build Replicates into the Approval Plan

Prepare independent reference and candidate pastes, rather than taking repeated readings only from one cup. Use coded fabric specimens and alternate the printing order to reduce operator and time effects. Record every result, including failed prints, with the same acceptance criteria.

Separate three sources of variation: repeated measurement on one specimen, independent paste preparation, and a later production lot. A good result at the first level does not prove the other two. Set the number of replicates and decision rule according to process risk and the method’s repeatability; this guide does not prescribe a universal sample count.

Liên hệ nhanh

Gửi yêu cầu của bạn

hoặc

Mẫu thử miễn phí · Trả lời trong vòng 24 giờ

Thắc mắc về sản phẩm & Hỗ trợ

Gửi yêu cầu về sản phẩm của bạn

Vui lòng cung cấp tên sản phẩm, ứng dụng, số lượng, điểm đến và bất kỳ tài liệu kỹ thuật (TDS), hình ảnh mẫu hoặc tài liệu nào mà quý khách đã có. FSX Chemical sẽ xem xét thông tin này và đề xuất bước tiếp theo liên quan đến báo giá, đối chiếu mẫu hoặc lựa chọn sản phẩm.

Thông tin sản phẩm Tên sản phẩm, cấp loại, mẫu mã, ảnh nhãn mác hoặc mã tham chiếu của nhà cung cấp.
Các tài liệu có sẵn TDS, SDS, COA, ảnh mẫu, danh mục sản phẩm hoặc dữ liệu thử nghiệm.
Chi tiết đơn hàng Số lượng dự kiến, hình thức đóng gói, nước nhập khẩu, cảng hoặc điều kiện thương mại.
Yêu cầu hoặc Vấn đề Quy trình in trên vải, yêu cầu về công thức, vấn đề hiện tại hoặc chỉ tiêu hiệu suất.