Why Acrylic Thickener Foams in Pigment Printing: Mixing, Surfactants and Defoamer Compatibility
Foam in pigment printing is rarely caused by acrylic thickener alone. It usually develops when mechanical air entrainment meets a surface-active formulation containing pigment dispersants, binder surfactants, wetting agents, acrylic rheology modifiers and other auxiliaries. Acrylic thickener can influence how bubbles form, move and collapse because it changes viscosity, yield behavior and—especially in HASE systems—associative interactions with surfactants and binder particles. The correct troubleshooting approach is therefore to separate air entrainment from stable foam, identify which addition step increases bubble persistence, evaluate the complete surfactant package, and select a defoamer that removes macro- and microfoam without damaging viscosity, screen transfer, leveling, print definition or cured-fabric quality.
Why Does Acrylic Thickener Foam in Pigment Printing?
Acrylic thickener does not usually create foam by itself.
Foam forms when air is introduced into the printing paste and the liquid contains enough surface-active material to stabilize that air.
A typical pigment-printing system contains:
- Pigment dispersants
- Binder emulsifiers
- Wetting agents
- Defoamers
- Fixers
- Acrylic thickener
During mixing, pumping or circulation, air can become dispersed through the paste.
If surfactants stabilize the bubble interfaces and the paste rheology slows bubble rise and collapse, persistent foam develops.
The practical mechanism is:
Mechanical Air Entrainment + Surface-Active Chemistry + Bubble-Stabilizing Rheology = Persistent Foam
The solution should therefore target the real cause rather than simply adding more defoamer.
Air Entrainment vs. Stable Foam
Not every bubble problem is the same.
Air Entrainment
Mechanical mixing traps air inside the paste.
The bubbles may disappear quickly once mixing stops.
Stable Foam
Surface-active molecules stabilize the air-liquid interface and prevent rapid bubble collapse.
The foam remains after mixing stops or reforms easily during pumping.
Microfoam
Very small bubbles remain suspended inside the viscous paste and can be difficult to see.
Microfoam can be more damaging than visible surface foam because it can:
- Distort viscosity measurements
- Reduce effective paste density
- Create pinholes or incomplete deposits
- Cause uneven screen transfer
Before changing chemistry, determine which foam type is present.
Where Does the Foam Come From?
A practical root-cause map includes four groups:
| Source | Typical Cause | First Check |
|---|---|---|
| Mechanical | High-speed mixing, vortex, pump suction | Mixing and circulation |
| Surface chemistry | Pigment/binder surfactants | Ingredient-by-ingredient addition |
| Rheology | High viscosity slows bubble release | Thickener dosage / shear profile |
| Defoamer mismatch | Too compatible or too incompatible | Defoamer grade / addition point |
More than one source can occur at the same time.
1. High-Shear Mixing and Air Entrainment
High-speed mixing is one of the most common physical causes of foam.
Air is pulled into the paste when:
- A deep vortex forms.
- The mixer blade is too close to the surface.
- The tank is under-filled.
- The pump draws air.
- Ingredients are added in a way that increases splashing.
The first troubleshooting step should therefore be mechanical.
Check:
- Mixer speed
- Blade position
- Tank fill level
- Vortex depth
- Pump seals / suction
- Return-line position
Reducing unnecessary air entrainment is usually cheaper and more reliable than trying to destroy every bubble chemically after it forms.
2. Pigment and Binder Surfactants
Water-based pigment and binder systems normally contain surfactants or dispersants.
These materials help:
- Stabilize pigment particles
- Stabilize binder emulsions
- Improve wetting
- Maintain colloidal stability
But the same surface-active molecules can also stabilize air bubbles.
This is why one pigment color or one binder supplier can produce more foam than another even when the thickener dosage is unchanged.
When foam changes after a raw-material change, check the full surfactant package before blaming the acrylic thickener.
3. How Acrylic Thickener Changes Bubble Stability
Acrylic thickener affects foam mainly through rheology.
Higher low-shear viscosity can:
- Slow bubble rise
- Slow drainage from the foam film
- Keep microbubbles suspended
Shear thinning can reduce apparent viscosity during mixing. Air entrainment still depends on mixing geometry, the vortex and the surface-active formulation; a flow curve alone does not predict how much air will enter.
When shear falls, apparent viscosity can rise. Any time-dependent structural recovery must be measured separately; its rate is not established by shear thinning alone. Bubble release depends on both the formulation and its flow and recovery behavior.
A possible, grade-dependent sequence is:
Mixing introduces air → flow and recovery affect bubble movement → check foam persistence, density and printing under defined conditions
Therefore, a thickener with excellent screen rheology can still require careful foam control.
4. Why HASE Systems Can Be More Sensitive to Surfactant Balance
HASE thickeners use hydrophobic associative groups in addition to pH-driven swelling.
Those hydrophobic groups can interact with:
- Binder particles
- Surfactants
- Pigment-dispersion components
- Some defoamer chemistries
Changing the surfactant balance can therefore alter both:
- Rheology
- Foam behavior
A new defoamer that works well in a non-associative ASE system may change the rheology of a HASE system more strongly.
Do not select defoamer independently from thickener architecture.
5. Pigment Dispersion and Dark-Shade Foam
Dark shades usually contain more pigment dispersion.
Higher pigment loading can increase:
- Surfactant concentration
- Dispersant concentration
- Water introduced with pigment
- Mixing demand
This can make dark shades foam more strongly than light shades.
If the problem occurs only in dark colors, compare:
- Pigment dosage
- Pigment supplier
- Mixing time
- Defoamer demand
Do not automatically increase thickener because the dark shade looks less dense or more aerated.
6. Binder Addition and Foam Persistence
Binder emulsion can change foam in several ways.
It may add:
- Surfactants
- Polymer particles
- Electrolytes
- Additional water
Some binder systems strongly stabilize foam; others collapse foam more readily.
A useful diagnostic is:
Thickener Base → Measure Foam → Add Pigment → Measure → Add Binder → Measure
If foam increases mainly after binder addition, the binder/surfactant package becomes the main investigation point.
7. Neutralizer and pH Effects
Neutralization can change:
- Acrylic-thickener viscosity
- Surfactant behavior
- Foam drainage
- Bubble release
If pH is too low, the thickener may not build enough viscosity.
If viscosity then rises rapidly after neutralization, bubbles introduced earlier can become trapped.
Neutralizer addition can also create foam if it is added with excessive splashing or high-speed mixing.
Control:
- Addition rate
- Mixing
- Final pH
- Rest time before foam evaluation
8. What Does a Defoamer Actually Do?
A defoamer destabilizes the foam film so bubbles can collapse or coalesce.
A good pigment-printing defoamer should:
- Suppress newly forming foam
- Break existing macrofoam
- Help remove persistent microfoam
- Remain effective through mixing and holding
- Avoid damaging binder or thickener compatibility
- Avoid creating print-surface defects
The balance is important.
If a defoamer is too compatible with the aqueous formulation, it may lose defoaming efficiency.
If it is too incompatible, it can create:
- Cratering
- Surface defects
- Separation
- Uneven wetting
Therefore, compatibility and defoaming strength must be optimized together.
Macrofoam vs. Microfoam
Macrofoam
Large visible bubbles or a foam layer on the paste surface.
Often easy to observe and relatively easy to knock down.
Microfoam
Small bubbles dispersed inside the paste.
Potential symptoms include:
- Milky or unusually opaque paste
- Apparent viscosity inconsistency
- Density loss
- Pinholes
- Uneven deposit
One defoamer can be effective against visible surface foam but weaker against microfoam.
Therefore, evaluate both visible foam and paste density / print quality.
Why Defoamer Compatibility Matters
The defoamer exists inside the same formula as:
- Acrylic thickener
- Binder
- Pigment dispersion
- Surfactants
Its chemistry can therefore change:
- Wetting
- Rheology
- Binder-film uniformity
- Print surface
Commercial water-based defoamer portfolios specifically distinguish products for:
- High-surfactant pigment concentrates
- High-shear processing
- Different acrylic binder systems
This shows why “one universal defoamer” is not a reliable formulation strategy.
Silicone vs. Non-Silicone Defoamer Routes
Silicone-based defoamers can be highly effective in water-based pigment systems and are widely used where strong foam knockdown is needed.
Non-silicone routes can include:
- Mineral-oil-based systems
- Polyether or polymeric systems
- Other hydrophobic defoaming technologies
Selection should consider:
- Foam knockdown
- Microfoam removal
- Binder compatibility
- Surface-defect risk
- Long-term persistence
- Local regulatory / customer requirements
Do not choose by chemistry name alone.
Where Should Defoamer Be Added?
Possible addition points include:
- Early in pigment / thickener preparation
- During binder let-down
- Final viscosity adjustment stage
- Controlled post-addition if foam appears during holding
Early addition can help prevent foam from becoming trapped during high-shear mixing.
Later addition can be useful when the final surfactant package has already formed.
Some commercial defoamers are designed specifically for high-shear early-stage use; others are selected for later-stage compatibility.
Use the defoamer supplier’s guidance and confirm performance in the actual paste.
How Much Defoamer Should Be Used?
There is no universal dosage.
Build a dosage ladder around the supplier-recommended range.
For each point, record:
- Visible foam height
- Foam collapse time
- Paste density if available
- Viscosity
- Screen performance
- Surface defects
The optimum dosage is:
Minimum Defoamer Needed for Stable Foam Control Without Negative Side Effects.
Do not maximize defoamer dosage.
What Happens When Too Much Defoamer Is Used?
Excess defoamer can create:
- Surface defects
- Cratering
- Uneven wetting
- Compatibility problems
- Changed rheology
- Print nonuniformity
This is why strong defoaming performance must be balanced with formula compatibility.
If foam disappears but print quality worsens, the system is not optimized.
Defoamer vs. Rheology: Why Viscosity Can Change
In associative acrylic systems, some defoamers can interact with hydrophobic regions in the rheology network.
This can change:
- Low-shear body
- Medium-shear viscosity
- Recovery
- Elasticity
Even in non-associative systems, defoamer can change the surfactant balance and therefore influence apparent viscosity.
Always measure viscosity after the final defoamer dosage is selected.
Foam Control Pass ≠ Rheology Pass.
How Foam Affects Screen Printing
Foam and trapped air can interfere with:
- Screen filling
- Squeegee transfer
- Solid-area coverage
- Fine-line definition
- Paste deposit
A bubble reaching the screen can temporarily block the normal liquid path.
Microfoam can also reduce the amount of actual liquid transferred per unit volume of paste.
Therefore, screen defects can appear even when the nominal paste viscosity is correct.
Typical Foam-Related Print Defects
Possible foam-related defects include:
- Pinholes
- White spots
- Uneven solid areas
- Patchy color
- Incomplete screen transfer
- Variable penetration
- Beginning-to-end shade inconsistency
These defects can also have other causes.
Do not diagnose foam from appearance alone.
Confirm with:
- Foam observation
- Paste density where available
- Deaerated control sample
- Controlled defoamer trial
Foam During Holding and Recirculation
A paste can look foam-free immediately after preparation but develop foam during:
- Pumping
- Recirculation
- Repeated stirring
- Long holding
Measure:
- Fresh foam
- Foam after controlled circulation
- Foam after holding
- Viscosity / pH at the same stages
A defoamer that works only immediately after preparation may not provide adequate long-run control.
Rotary Screen: Continuous-Shear Foam Risk
Rotary-screen printing can expose the paste to continuous pumping and repeated shear.
This increases the importance of:
- Pump suction integrity
- Return-line design
- Long-term defoamer persistence
- Continuous-shear rheology
A paste that is stable in a short beaker test can foam after repeated circulation.
Rotary qualification should therefore include a recirculation simulation or production trial.
Flat Screen: Stroke and Pause Effects
Flat-screen printing exposes the paste to repeated squeegee strokes with pauses between them.
Foam can collect:
- At the screen edge
- In low-flow zones
- After repeated manual or mechanical stirring
Check whether foam increases after pause/restart cycles.
Do not evaluate only the first few strokes.
How to Build a Reproducible Foam Diagnostic Test
Use a controlled comparison of the complete pigment paste. The following is a suggested diagnostic workflow, not FSX trial data or a universal acceptance standard.
1. Control the preparation and mixing history
Keep formula, batch mass, temperature, paste age and ingredient addition sequence consistent. Record vessel diameter, fill level, impeller type and diameter, immersion depth, speed and mixing time. The same rpm on different equipment does not reproduce the same mixing conditions. Use mixing conditions relevant to production and compatible with the binder and additives; do not impose damaging high shear merely to create more foam.
2. Prepare a composition-matched low-air reference
Use the same formulation and temperature, prepared to minimize air while still achieving adequate dispersion. If using a de-airing method, confirm that it does not remove volatile components, concentrate the paste or damage the emulsion. Do not add water to make the reference easier to de-air. Record the procedure and the time between preparation and measurement.
3. Measure visible foam and density separately
Compare foam height only in vessels with the same geometry and fill level, at defined times after mixing. Record bubble persistence and collapse as well as initial height. Surface foam alone does not measure air dispersed throughout the paste.
For a density check, use a clean, calibrated fixed-volume cup and a balance suitable for the sample mass. Tare the cup, follow the same filling and leveling procedure, and divide net paste mass by cup volume. Repeat with fresh fills at the same temperature and elapsed time; record results rather than accepting a single reading.
For otherwise identical paste, lower measured density relative to the low-air reference is consistent with greater entrained air. It is not proof if formulation, solids, temperature or sampling differs. A reference that still contains air cannot establish absolute air content. Use density alongside bubble observations and printing tests.
| Observation | Check next | Avoid concluding |
|---|---|---|
| Surface foam falls but density remains low | Dispersed bubbles, reference preparation and cup-filling repeatability | All air has been removed |
| Foam increases after an ingredient addition | A matched trial controlling addition shear, temperature and concentration | The ingredient’s surfactant chemistry is the only cause |
| Density recovers but craters appear | Defoamer dispersion, dose, compatibility and possible contamination | Foam control alone makes the paste acceptable |
| Pinholes persist with low-air paste | Fabric wetting, screen condition, contamination and drying or curing conditions | Every pinhole is a foam defect |
4. Confirm performance after holding and circulation
Repeat the comparison after the intended holding period and relevant circulation conditions. Print the same fabric under matched settings, then complete the specified curing cycle and quality tests. Approve the treatment only when foam control, paste flow and finished-print requirements are all met.
Build a Stage-by-Stage Foam Map
| Stage | Record | Main Question |
|---|---|---|
| Water + Thickener | Foam / density | Does the thickener base trap air? |
| After Neutralization | Foam / viscosity | Did activation trap existing air? |
| After Pigment | Foam / viscosity | Did pigment surfactants increase foam? |
| After Binder | Foam / viscosity | Did binder surfactants stabilize foam? |
| After Defoamer | Foam / rheology | Did foam fall without damaging paste behavior? |
| After Holding | Foam / viscosity | Is the control persistent? |
This map is often more useful than one final foam observation.
Build a Defoamer-Dosage Curve
Include the current approved formula as a control. Test candidate levels within the defoamer supplier’s recommended range and incorporation procedure. State whether dosage is mass percent of as-supplied defoamer in final paste or an active-content basis; these are not interchangeable. Keep the final batch mass consistent and account for carrier water when comparing preparations.
At each level, record incorporation stage and mixing conditions, foam height over time, density, viscosity method, flow recovery and print defects. Repeat after holding and circulation. Select a working window that meets the mill’s agreed limits, rather than choosing the dose that gives the lowest foam height in one beaker.
Compatibility evidence: BYK’s technical discussion of silicone defoamers explains that compatibility and incorporation affect defoaming and crater formation. Those coating examples explain the trade-off; they do not validate a particular defoamer, dosage or FSX textile formulation. Confirm performance in the actual pigment paste and cured print.
Production Trial Approval
Run the best laboratory foam-control condition on the real machine.
Record:
- Thickener grade / batch
- Thickener dosage
- Defoamer grade / dosage
- Addition point
- Mixing condition
- Paste pH
- Start / mid / end-run viscosity
- Visible foam
- Machine speed
- Screen behavior
- Print uniformity
- Color consistency
- Curing result
Approve a defoamer package only when foam control remains stable across the intended production window.
Common Foam Troubleshooting Mistakes
1. Blaming the Thickener First
Foam usually comes from the whole surfactant and mixing system.
2. Adding More Defoamer Before Checking Mixing
Mechanical air entrainment may be the main problem.
3. Judging Only Visible Surface Foam
Microfoam can remain inside the paste.
4. Selecting Defoamer by Foam Knockdown Only
Compatibility and print-surface defects also matter.
5. Ignoring HASE Interaction
Associative thickener can respond to hydrophobic defoamer and surfactant chemistry.
6. Testing Defoamer in Water Instead of Complete Paste
The real binder/pigment surfactant package determines foam behavior.
7. Using One Defoamer Dosage for Every Shade
High-pigment dark shades can have a higher surfactant load.
8. Ignoring Long-Run Recirculation
Foam can develop after repeated pumping even when the fresh paste looks stable.
Troubleshooting Table
| Observed Problem | First Variables to Check | Do Not Assume |
|---|---|---|
| Foam appears during high-speed mixing | Vortex, blade position, tank fill, surfactants | The thickener is inherently foamy |
| Foam increases after pigment | Pigment surfactant/dispersant load | More defoamer is the only fix |
| Foam increases after binder | Binder emulsifier package, dilution, mixing | Binder is incompatible with thickener |
| Visible foam disappears but print has pinholes | Microfoam, density, deaeration | Surface foam control is enough |
| Defoamer removes foam but viscosity changes | Associative rheology / surfactant balance | Defoamer has no rheological effect |
| Defoamer causes craters or poor wetting | Overdose, incompatibility, addition point | Stronger defoamer is always better |
| Rotary paste foams after long circulation | Pump suction, recirculation, defoamer persistence | Fresh lab foam test proves long-run stability |
| Dark shades foam more than light shades | Pigment loading / surfactant package | One defoamer dose fits every color |
Total Cost in Use
Foam creates hidden cost through:
- Extra defoamer
- Longer mixing / deaeration
- Reduced machine speed
- Screen defects
- Rework
- Rejected prints
A useful model is:
Cost per accepted m² = allocated monetary process cost for the production lot ÷ accepted finished fabric area.
Use the same production boundary, currency and final quality requirements for each foam-control option; for example, paste preparation through curing and final inspection. Price actual paste-material consumption, including thickener and defoamer, as kilograms consumed multiplied by delivered price per kilogram. Include consistently allocated mixing, deaeration, printing, curing and cleaning costs.
Convert measured labor or equipment time with declared hourly rates and energy with measured consumption and tariffs. Count additional rework, disposal and reject-related costs only where they are not already included in materials or operating charges. Do not add a second downtime charge when the same occupied hours are covered by the equipment rate. Record efficiency and interruption time separately if no defensible monetary allocation is available; do not add a percentage or hours directly to currency.
A more compatible thickener/defoamer pair can justify a higher material price if it reduces:
- Foam correction
- Machine interruptions
- Pinholes
- Batch variability
Divide by accepted finished fabric area after the agreed quality checks. Use the same accounting boundary for both options; a cost per linear metre comparison also requires matched fabric width. Defoamer price per kilogram alone cannot establish the lower-cost process.
What Information Should You Send to a Thickener Supplier?
For foam troubleshooting, provide:
- Current acrylic thickener / TDS
- Thickener dosage
- ASE / HASE information if known
- Neutralizer and final pH
- Pigment dispersion and dosage
- Binder grade and dosage
- Current defoamer and dosage
- Mixing speed / equipment
- Batch size
- Flat or rotary screen
- Holding / circulation time
- Stage where foam first increases
- Observed print defect
FSX Chemical can use this information through Samples & Matching to define a controlled thickener / formulation comparison.
Review Synthetic Printing Thickeners and Textile Printing Thickener Applications for process-based product matching.
How Should a Mill Troubleshoot Foam in Acrylic Pigment Paste?
A practical sequence is:
Check Mechanical Air Entrainment → Build Stage-by-Stage Foam Map → Identify Pigment / Binder Surfactant Effect → Confirm Thickener Rheology → Test Defoamer Compatibility → Build Dosage Curve → Hold / Recirculate → Screen Print → Approve Production Window
The key principles are:
- Foam usually comes from the interaction of mixing, surfactants and rheology rather than acrylic thickener alone.
- Visible surface foam and microfoam should be treated as different diagnostic problems.
- HASE-type associative thickeners can be more sensitive to changes in surfactant and hydrophobic defoamer chemistry.
- Select a defoamer with a suitable compatibility–defoaming balance that controls foam without damaging rheology or print quality. Maximum compatibility alone is not the target.
- Dark shades, high-shear mixing and long rotary circulation can require more demanding foam-control validation.
- The final decision should be based on stable screen printing and Total Cost in Use, not foam height alone.
Frequently Asked Questions
1. Does acrylic thickener itself cause foam?
Usually not by itself. Foam typically develops when mechanical mixing introduces air into a surfactant-containing pigment/binder system, while the thickener rheology helps keep bubbles suspended.
2. Why does foam increase after pigment is added?
Pigment dispersions contain surfactants and dispersants that can stabilize bubbles, especially at high pigment loading.
3. Why does binder make the paste foam more?
Binder emulsions contain surfactants and polymer particles that can change both bubble stability and thickener rheology.
4. Why can HASE thickener be sensitive to defoamer chemistry?
HASE uses hydrophobic associative interactions, so surfactants and hydrophobic defoamer components can alter the rheological network.
5. What is microfoam?
Microfoam is very small trapped air bubbles dispersed through the paste. It may not create a visible foam layer but can affect density, viscosity measurement and print uniformity.
6. Should I increase defoamer dosage until all bubbles disappear?
No. Excess defoamer can cause wetting, cratering, compatibility or rheology problems. Use the minimum dose that gives stable foam control without print defects.
7. Is silicone defoamer always best?
No. Silicone systems can be very effective, but the best chemistry depends on binder, surfactants, thickener architecture and print-surface requirements.
8. When should defoamer be added?
The best addition point is product- and process-specific. Some defoamers work best during high-shear preparation; others are selected for later let-down or post-addition.
9. Why does the paste foam more during rotary-screen circulation?
Continuous pumping, suction leaks, return-line turbulence and repeated shear can keep introducing air and challenge defoamer persistence.
10. Why are dark pigment shades more foamy?
Higher pigment loading usually introduces more surfactant/dispersant and can require longer or stronger mixing.
11. Can defoamer change viscosity?
Yes. It can change surfactant balance and, in associative acrylic systems, interact with the rheological network. Always recheck viscosity after defoamer optimization.
12. What should I send FSX Chemical for foam troubleshooting?
Send the current thickener/TDS, dosage, pigment, binder, pH, defoamer, mixing equipment, batch size, machine route, circulation time and the stage where foam first becomes excessive.
Control Foam Without Sacrificing Pigment-Paste Rheology
If your pigment-printing paste traps air during mixing, develops persistent foam after pigment or binder addition, or shows pinholes and uneven transfer after defoamer adjustment, FSX Chemical can help structure a controlled thickener and formulation review.
For a useful technical review, send:
- Your current acrylic thickener sample, TDS or COA
- Thickener dosage
- Neutralizer and final pH
- Pigment dispersion and dosage
- Binder grade and dosage
- Current defoamer grade / dosage
- Mixing equipment and batch size
- Flat or rotary screen route
- Holding / circulation time
- Observed foam and print defect
Start with Samples & Matching for a controlled current-vs-candidate comparison.
Review Synthetic Printing Thickeners for the current FSX synthetic printing range.
You can also Request a Factory-Direct Quote after the suitable grade and working formulation are confirmed or Contact FSX Chemical for technical discussion📧 Email: Service@fsxchemical.com
The most effective foam-control strategy is not simply more defoamer. First reduce unnecessary air entrainment, identify which surfactant-rich ingredient stabilizes the bubbles, then select a defoamer that remains compatible with the acrylic thickener, binder and screen-printing rheology.
Related posts
Textile Printing Thickeners by Dye and Printing Process
Cellulose-Based Textile Printing Paste: CMC Grade and Supplier Evaluation
Sodium Alginate vs CMC for Textile Printing: Performance and Cost Comparison
How to Choose the Right Textile Printing Thickener for Your Fabric
Textile Printing Chemicals and Their Functions: 10 Key Groups
Textile Printing Thickeners Compared: Sodium Alginate, CMC, CMS and Digital Paste
Digital Textile Printing Paste Selection: Reactive, Disperse and Pigment Systems
Evaluating FSX Digital Printing Paste: Product Fit, Trial Evidence and Supply Checks
Digital Textile Printing Paste Stability: 10 Process Controls
FSX Digital Fabric Pretreatment: A Buyer Evaluation Guide
Exploring New Textile Chemical Solutions for Digital Inkjet Printing
Textile Printing Chemical Innovations: Five Directions to Evaluate
Quick Links
Send Your Product Requirement
Share the product name, application, quantity, destination and any TDS, sample photo or document you already have. FSX Chemical will review the information and recommend the next step for quotation, sample matching or product selection.