How to Measure Electrolyte Tolerance of a Synthetic Thickener for Pigment Printing

Electrolyte tolerance should be measured as viscosity and rheology retention under a clearly defined ionic...

Electrolyte tolerance is one of the most important performance properties of a synthetic thickener because a grade that builds high viscosity in clean water can lose much of its thickening efficiency after pigment, binder, fixer, hard-water ions or other auxiliaries are introduced. A useful test should therefore measure viscosity retention under controlled ionic stress rather than compare water viscosity alone. The most reliable qualification uses three levels: a simple reference-salt screening test, targeted challenges with relevant ions such as calcium or magnesium when needed, and final verification in the complete pigment-printing paste. pH, temperature, thickener dosage, salt basis, mixing sequence and equilibration time must be standardized before one grade is described as more electrolyte-tolerant than another.

How Do You Measure Electrolyte Tolerance of a Synthetic Thickener?

The simplest useful method is to measure how much viscosity remains after a controlled amount of electrolyte is added to a standardized thickener system.

A practical calculation is:

Viscosity Retention (%) = Viscosity After Electrolyte ÷ Initial Viscosity × 100

But the number is meaningful only if the test also fixes:

  • ঘনকারী মাত্রা
  • চূড়ান্ত pH
  • Water quality
  • Salt type
  • Salt concentration basis
  • Mixing method
  • Equilibration time
  • পরিমাপের তাপমাত্রা
  • Instrument / spindle / speed / reading time

A good qualification process uses:

Reference Salt Screening → Relevant-Ion Challenge → Complete Pigment-Paste Verification

This prevents a high water-viscosity grade from being incorrectly described as electrolyte-tolerant before it is tested in the real formulation.

Why Electrolyte Tolerance Matters in Pigment Printing

Acrylic synthetic thickeners are usually evaluated first in water because this makes thickening efficiency easy to see.

Production paste is much more complex.

It can contain:

  • Pigment dispersions
  • Binder emulsions
  • Fixers
  • আর্দ্রকারী পদার্থ
  • ডিফোমার
  • Hard-water ions
  • Neutralizer salts

These ingredients can change ionic strength and polymer interaction.

A grade that gives excellent water viscosity may therefore show:

  • Large viscosity loss
  • Slow viscosity drift
  • Different recovery
  • Poor screen behavior

inside the complete printing paste.

Electrolyte tolerance should therefore be treated as a separate performance property from water thickening efficiency.

Why Electrolytes Change Acrylic-Thickener Viscosity

Many synthetic acrylic thickeners contain ionized carboxylate groups after neutralization.

Those negative charges help keep the polymer chains expanded in water.

A simplified mechanism is:

Neutralization → Negative Charge → Electrostatic Repulsion → Polymer Expansion → Viscosity

When salts are added, dissolved ions can reduce the effective repulsion between charged polymer segments.

A simplified salt response is:

Electrolyte ↑ → Charge Screening ↑ → Polymer Expansion Can Decrease → Viscosity Can Fall

The magnitude depends on polymer architecture, salt type, concentration, pH and the rest of the formulation.

অতএব:

Water Viscosity ≠ Electrolyte Tolerance.

ASE vs. HASE: Why Salt Response Can Differ

ASE-type thickeners rely strongly on alkali swelling, chain expansion and hydrodynamic volume.

HASE thickeners add hydrophobic associative interactions.

Salt can therefore affect HASE through more than one route:

  • Charge screening
  • Polymer conformation
  • Hydrophobic association
  • Surfactant structure
  • Binder interaction

Published HASE studies show that increasing salt concentration can reduce viscosity and change viscoelastic behavior, but the magnitude depends strongly on hydrophobe architecture and shear conditions.

অতএব:

HASE ≠ Automatically More Salt-Tolerant.

Test the actual commercial grade.

Where Do Electrolytes Enter a Pigment Paste?

Potential sources include:

  • Pigment-dispersion salts and dispersants
  • Binder-emulsion components
  • Cationic or ionic fixers
  • নিরপেক্ষকারী প্রতিআয়ন
  • Calcium / magnesium from hard water
  • Other textile auxiliaries

The total ionic environment can therefore increase even when no ingredient is described simply as “salt.”

This is why electrolyte tolerance should be evaluated in stages.

Electrolyte Tolerance Is Not One Universal Number

A statement such as:

“This thickener tolerates 2% salt.”

is incomplete unless it also specifies:

  • Which salt?
  • 2% based on what mass?
  • What thickener concentration?
  • What pH?
  • What temperature?
  • What initial viscosity?
  • How long after salt addition?
  • What viscosity method?

Different laboratories can obtain very different “salt tolerance” values if these conditions are not standardized.

Use electrolyte tolerance as a defined test method, not a marketing adjective.

A Three-Level Electrolyte-Tolerance Test

LevelTest SystemPurpose
1Thickener + water + reference saltCompare intrinsic salt response
2Thickener + relevant Ca/Mg or process waterCheck plant-water robustness
3Complete pigment / binder / fixer pasteConfirm real production compatibility

All three levels answer different questions.

Do not use Level 1 to replace Level 3.

Level 1: Reference-Salt Screening

Reference-salt screening is useful for comparing several candidate synthetic thickeners under one controlled ionic challenge.

Use:

  • Same water
  • Same thickener dosage
  • Same activation method
  • Same pH
  • Same salt
  • Same temperature
  • Same measurement method

Measure the no-salt baseline first.

Then add defined salt levels and measure viscosity retention.

The result provides a relative comparison between candidates.

Which Salt Should Be Used for Screening?

Sodium chloride is often useful as a simple monovalent reference electrolyte because it is easy to prepare reproducibly and creates a straightforward ionic challenge.

However:

NaCl Screening ≠ Complete Pigment-Paste Simulation.

If the suspected production problem is:

  • Hard water
  • Calcium-rich process water
  • Magnesium-rich process water
  • A specific ionic fixer

then the next test should reproduce that relevant chemistry.

Use the reference salt for ranking, then use process-relevant ions for qualification.

Define the Concentration Basis Before Testing

Salt concentration can be reported on different bases.

Examples include:

  • Percentage of total test mass
  • Percentage relative to water phase
  • Mass per liter
  • Molar concentration

Pick one method and use it consistently.

For factory QC, a mass-based method can be convenient.

For scientific comparison between different salts, molar concentration or ionic strength can provide a more meaningful comparison.

Do not compare two test reports until the concentration basis is confirmed.

Build a Controlled Salt-Concentration Ladder

Do not test only:

0 Salt vs. One High-Salt Point.

Use several points across the relevant operating or stress range.

প্রতিটি পয়েন্টের জন্য রেকর্ড করুন:

  • Salt type
  • Salt level
  • চূড়ান্ত pH
  • সান্দ্রতা
  • সান্দ্রতা ধরে রাখা
  • দৃষ্টি
  • Foam / gel if present

কাহিনী:

Electrolyte Level → Viscosity Retention

The curve is more informative than one pass/fail point.

It can show:

  • Gradual loss
  • Stable region
  • Sharp collapse threshold

Use process-relevant levels rather than copying arbitrary concentrations from an unrelated industry.

Calculate Viscosity Retention

A useful internal calculation is:

Viscosity Retention (%) = Vsalt ÷ V0 × 100

where:

  • V0 = viscosity before electrolyte challenge
  • Vsalt = viscosity after the defined electrolyte challenge

This normalizes candidates with different starting viscosities.

For example, a candidate with slightly lower baseline viscosity can still be more robust if it retains a much larger fraction of its initial viscosity after the same salt challenge.

But retention alone is not enough.

Also evaluate:

  • Absolute final viscosity
  • রিওলজি
  • Screen result

Control pH Before Comparing Salt Tolerance

pH-responsive acrylic thickeners must be compared at the correct activation condition.

If Candidate A is fully activated and Candidate B is under-neutralized, the test does not measure salt tolerance fairly.

রেকর্ড:

  • pH before salt
  • pH after salt
  • pH after holding

Use each grade within its validated operating range.

Do not force every product to the same arbitrary pH if the suppliers specify different useful activation windows.

The correct comparison is:

Each Grade Correctly Activated → Same Defined Electrolyte Challenge.

Control Temperature and Measurement Method

Every electrolyte-tolerance result should record:

  • তাপমাত্রা
  • যন্ত্র
  • স্পিন্ডল / রোটর
  • গতি
  • পড়ার সময়

A salt test measured at one temperature cannot be compared reliably with another sample measured at a different temperature.

FSX Chemical’s current thickener-testing guidance uses the same principle: viscosity becomes meaningful only when the measurement method is standardized.

Keep all candidate samples at the same test temperature before calculation.

Control Mixing and Equilibration Time

Viscosity can change during and after salt addition.

Standardize:

  • Salt-solution concentration
  • Addition rate
  • Mixing speed
  • Mixing time
  • Rest / equilibration time

If concentrated salt solution is poured into a thickener-rich zone, the local ionic concentration can be much higher than the final average.

This can create a stronger apparent shock than a well-mixed gradual addition.

Use the same addition procedure for every candidate.

Level 2: Calcium, Magnesium and Process-Water Challenge

If the mill uses hard water or sees factory-to-factory variation, the next test should include relevant hardness ions or real process water.

তুলনা করুন:

  • Low-hardness reference water
  • Normal plant water
  • Representative harder-water challenge

If deeper diagnosis is needed, separate calcium and magnesium challenges.

Keep:

  • চূড়ান্ত pH
  • ঘনকারী মাত্রা
  • তাপমাত্রা
  • Measurement method

constant.

This reveals whether a grade that tolerates NaCl still struggles with divalent ions.

Why Monovalent and Divalent Ions Should Not Be Treated as Equivalent

Sodium is monovalent.

Calcium and magnesium are divalent.

Divalent ions can interact more strongly with anionic polymer and dispersant systems.

সম্ভাব্য প্রভাবগুলির মধ্যে রয়েছে:

  • Stronger charge screening
  • Polymer contraction
  • Changes in pigment dispersant behavior
  • Changes in binder colloidal stability

অতএব:

1% NaCl Test ≠ 1% CaCl2 Test.

The two salts do not provide the same molar concentration, ion valence or ionic strength.

Weight Percentage vs. Molar / Ionic Comparison

For production QC, weight percentage is often simple and practical.

For comparing fundamentally different salts, equal weight percentages can be misleading because:

  • Molecular weights differ.
  • The number of ions released differs.
  • Ion valence differs.

For technical R&D, consider comparing salts on:

  • Molar basis
  • Ionic-strength basis
  • Actual plant exposure basis

depending on the question.

For factory qualification, the most important test is still the real ionic environment the paste will see in production.

Level 3: Complete Pigment-Paste Verification

This is the production decision test.

Prepare the complete:

Water + Thickener + Pigment + Binder + Fixer + Auxiliaries

সিস্টেম।.

Measure:

  • Viscosity before each major addition
  • পিএইচ
  • চূড়ান্ত সান্দ্রতা
  • ধরা-সময়ের সান্দ্রতা
  • ফেনা
  • Gel / floc / separation
  • স্ক্রিন আচরণ

The complete paste may behave differently from the simple NaCl test because:

  • Surfactants affect HASE association.
  • Binder particles interact with associative thickeners.
  • Pigment dispersants contribute ionic and colloidal effects.
  • Fixers can create strong local charge effects.

Use Level 3 for commercial approval.

Binder as an Electrolyte / Compatibility Challenge

Binder does not act like pure salt, but it can change the ionic environment.

It can introduce:

  • জল
  • সারফ্যাকট্যান্টসমূহ
  • ইলেক্ট্রোলাইটসমূহ
  • পলিমার কণা
  • pH shift

If the paste loses much more viscosity after binder than after an equivalent water dilution, chemistry is contributing beyond simple dilution.

Use:

ঘনকারী + সমপরিমাণ জল

as a control against:

Thickener + Actual Binder.

Pigment Dispersion as a Formulation Challenge

Pigment dispersion can add:

  • বিস্তারক
  • সারফ্যাকট্যান্টসমূহ
  • লবণসমূহ
  • জল
  • Pigment particles

A dark shade usually introduces more of this package than a pale shade.

Therefore, electrolyte tolerance should be checked at representative:

  • Light pigment load
  • Normal pigment load
  • High / dark pigment load

if the plant uses a wide shade range.

Fixers and High-Ionic Auxiliaries

Fixers can create a strong ionic challenge even at a relatively small dosage.

If the fixer is cationic and the acrylic thickener is anionic, the problem may include both:

  • General electrolyte screening
  • Direct opposite-charge interaction

In that case, a simple NaCl curve cannot predict the complete behavior.

Test the real fixer at production-relevant levels and dilution conditions.

Addition Order and Local Electrolyte Shock

Electrolyte tolerance is affected by how the ionic ingredient enters the paste.

A concentrated salt or fixer solution poured into a poorly mixed thickener-rich zone can create:

  • Temporary extreme ionic strength
  • Local polymer contraction
  • Gel or floc
  • Irreversible-looking viscosity loss

For a fair test, standardize:

  • Pre-dilution
  • Addition rate
  • Feed point
  • মিশ্রণ

Production qualification should reproduce the actual addition method.

Holding-Time Viscosity Retention

Some electrolyte effects are immediate.

Others develop during holding.

রেকর্ড:

  • নতুন সান্দ্রতা
  • Intermediate viscosity
  • End-of-shift viscosity
  • পিএইচ
  • তাপমাত্রা
  • দৃষ্টি

Calculate viscosity retention both:

  • Immediately after challenge
  • After the relevant holding period

A grade that looks excellent at 10 minutes but collapses after several hours is not production-stable.

Measure Rheology, Not Only One Viscosity Value

Electrolytes can change:

  • Low-shear body
  • Shear thinning
  • Elasticity
  • Structural recovery

In HASE systems, salt can change the balance between electrostatic swelling and hydrophobic association.

অতএব:

High Viscosity Retention ≠ Complete Rheology Retention.

For important candidates, compare:

  • Low-speed viscosity
  • Higher-speed viscosity
  • Post-shear recovery
  • Stringing / release if relevant

Connect Electrolyte Tolerance to Screen Printing

The best electrolyte-tolerant grade is not the one with the highest retained beaker viscosity.

It should also maintain:

  • Screen transfer
  • সংজ্ঞা মুদ্রণ করুন
  • Controlled penetration
  • ঘন-ক্ষেত্রের সমতা
  • Stable running

A candidate can retain viscosity but become too elastic or stringy.

Another can lose some viscosity yet remain inside the useful printing window.

Production performance determines whether the retention level is acceptable.

  1. Select the thickener candidate and confirm the correct activation method.
  2. Prepare all candidates at one defined water quality and test temperature.
  3. Record baseline pH and viscosity.
  4. Prepare one reference salt stock solution.
  5. Build a controlled salt-concentration ladder.
  6. Use identical addition, mixing and equilibration conditions.
  7. Record pH and viscosity at every salt point.
  8. Calculate viscosity retention.
  9. Repeat selected candidates with process water / Ca / Mg if relevant.
  10. Repeat the most useful candidates in the complete pigment/binder/fixer paste.
  11. Check holding stability.
  12. Screen print and cure before final approval.

The method should be documented so incoming batches can be compared using the same procedure.

Synthetic Thickener Electrolyte-Tolerance Comparison Table

CandidateBaseline ViscositySalt ChallengeViscosity RetentionHeld RetentionComplete-Paste Result
Aরেকর্ডDefinedCalculateCalculatePass / Conditional / Fail
Bরেকর্ডDefinedCalculateCalculatePass / Conditional / Fail
Cরেকর্ডDefinedCalculateCalculatePass / Conditional / Fail

Do not rank candidates only from baseline viscosity.

A lower-baseline candidate can be better if it remains inside the production window after the complete electrolyte challenge.

How Should Acceptance Limits Be Set?

Do not use a universal rule such as:

“A good thickener must retain 80% viscosity.”

That threshold may be too strict for one process and too weak for another.

Set acceptance from:

  • Historical successful production
  • Actual pigment / binder / fixer formula
  • Required screen behavior
  • Measurement repeatability
  • Finished-print quality

A useful specification can include:

  • Minimum retained viscosity under the defined test
  • No gel / floc / separation
  • Acceptable holding drift
  • Acceptable screen performance

The specification belongs to the test method, not the product name alone.

Can Electrolyte Tolerance Be Used for Incoming QC?

Yes, after a commercial grade has been approved.

A practical incoming or periodic application check can use:

  • Reference water
  • Fixed thickener dosage
  • Fixed activation method
  • One defined electrolyte challenge
  • Standard pH / temperature / viscosity method

Compare the new batch with:

  • Approved reference batch
  • Retained sample
  • Validated control range

Do not use an incoming salt test as the only release criterion.

Also verify identity, appearance, solids, pH and other agreed QC parameters.

উৎপাদন পরীক্ষার অনুমোদন

After laboratory ranking, run the best candidate in the real pigment-printing process.

রেকর্ড:

  • ঘনকারী গ্রেড / ব্যাচ
  • ঘনকারী মাত্রা
  • Pigment / binder / fixer formula
  • Water quality
  • চূড়ান্ত pH
  • শুরু/মধ্য/শেষ-প্রবাহ সান্দ্রতা
  • Holding time
  • Machine type
  • Screen / squeegee conditions
  • সংজ্ঞা মুদ্রণ করুন
  • প্রবেশ
  • Color consistency
  • শুকনো/ভেজা ঘষা
  • কাপড়ের হাত

Approve the grade only if electrolyte tolerance translates into stable production performance.

Common Electrolyte-Tolerance Testing Mistakes

1. Testing Water Viscosity Only

High water viscosity does not prove salt tolerance.

2. Using One Salt Point Only

A concentration ladder reveals the stability region and collapse behavior.

3. Saying “2% Salt” Without Defining the Basis

The result cannot be reproduced unless the concentration basis is clear.

4. Comparing NaCl and CaCl2 at Equal Weight Percentage

The salts differ in molecular weight, ion valence and ionic strength.

৫. pH উপেক্ষা করা

Under- or over-activation can be mistaken for poor salt tolerance.

6. Measuring at Different Temperatures

Temperature changes apparent viscosity independently of electrolyte tolerance.

7. Ignoring Addition Order

Local electrolyte shock can exaggerate instability.

8. Calling a Grade Salt-Tolerant Before Complete-Paste Testing

Binder, pigment, fixer and surfactants can change the response significantly.

ত্রুটি সমাধান সারণি

Observed Resultপ্রথমে যাচাই করার ভেরিয়েবলসমূহঅনুমান করবেন না
Viscosity drops sharply after first salt pointpH, salt basis, activation, grade architectureThe test itself is correct
NaCl tolerance is good but plant paste still collapsesCa/Mg, binder, pigment, fixerNaCl predicts the complete formula
Ca/Mg challenge is much worse than NaClDivalent-ion sensitivityAll electrolytes are equivalent
Fresh retention is good but held viscosity fallsHolding chemistry, pH, temperatureImmediate retention proves production stability
Viscosity retained but screen release worsensElasticity, recovery, stringingRetention percentage defines printability
One binder causes much larger lossBinder electrolytes / surfactants / associationThe thickener alone is salt-sensitive
Diluted fixer is more stable than concentrated fixer additionLocal ionic / charge shockFinal dosage is the only relevant variable
Two labs report different salt toleranceSalt basis, pH, temperature, spindle, mixingThe products are necessarily inconsistent

ব্যবহারে মোট খরচ

Electrolyte tolerance affects cost through:

  • ঘনকারী মাত্রা
  • Formula correction
  • Water-treatment demand
  • Machine stability
  • পুনর্নির্মাণ
  • Quality loss

একটি উপকারী মডেল হল:

Total Cost in Use = Thickener + Water / Formula Control + Correction Additions + Machine Efficiency + Rework + Quality Loss

A higher-priced synthetic thickener can be more economical if it:

  • Retains viscosity at lower dosage
  • Handles the real binder/pigment ionic load better
  • Reduces correction additions
  • Improves long-run consistency

Compare the validated production cost, not only water viscosity or price per kilogram.

আপনি সরবরাহকারীকে কী তথ্য পাঠাবেন?

For useful electrolyte-tolerance matching, provide:

  • বর্তমান সিন্থেটিক ঘনকারী / মোট দ্রবীভূত পদার্থ
  • ঘনকারী মাত্রা
  • Activation method and pH
  • সান্দ্রতা এবং সম্পূর্ণ পরীক্ষণ পদ্ধতি
  • Current electrolyte-tolerance test method if any
  • Pigment product and dosage
  • Binder grade and dosage
  • Fixer / ionic auxiliaries
  • Water hardness / conductivity
  • Holding time
  • সমতল বা ঘূর্ণায়মান স্ক্রিন
  • Observed failure: viscosity loss, drift, floc, screen instability or cost

FSX কেমিক্যাল এই তথ্যটি ব্যবহার করতে পারে মাধ্যমে নমুনা ও মিলान to structure a controlled candidate comparison.

পর্যালোচনা সিন্থেটিক প্রিন্টিং ঘনকারী, টেক্সটাইল প্রিন্টিং থিকনার পরীক্ষার পরামিতি এবং Why Synthetic Printing Thickener Loses Viscosity After Pigment, Binder or Electrolytes সম্পর্কিত নির্বাচন লজিকের জন্য।.

How Should a Mill Define Electrolyte Tolerance for Synthetic Thickener?

একটি ব্যবহারিক নিয়ন্ত্রণ শৃঙ্খল হল:

Correctly Activate the Grade → Standardize Water / pH / Temperature → Build Reference-Salt Ladder → Calculate Viscosity Retention → Challenge Relevant Ca/Mg or Process Water → Test Complete Pigment/Binder/Fixer Paste → Hold → Screen Print → Define Production-Based Acceptance Limits

মূল নীতিগুলি হল:

  1. Electrolyte tolerance is a defined test result, not a generic product claim.
  2. Water viscosity and salt tolerance are separate thickener properties.
  3. NaCl is useful for controlled screening, but it does not reproduce every process electrolyte.
  4. Divalent ions such as calcium and magnesium should be challenged separately when hard water matters.
  5. pH, temperature, salt basis, mixing and equilibration must be standardized before candidates are compared.
  6. The commercially useful grade is the one that remains inside the complete-paste rheology and printing window at the lowest practical Total Cost in Use.

প্রায়শই জিজ্ঞাসিত প্রশ্নাবলী

1. What is electrolyte tolerance in a synthetic thickener?

It is the ability of the thickener to maintain useful viscosity and rheology when dissolved ions or ionic formulation components are present.

2. How do I calculate viscosity retention?

Divide the viscosity after the defined electrolyte challenge by the initial viscosity and multiply by 100. Use the same temperature and test method for both readings.

3. Is sodium chloride a good salt for electrolyte-tolerance testing?

It is useful as a reproducible monovalent reference salt, but it does not replace testing with hard-water ions, binder, pigment or fixer when those are the real production stresses.

4. What salt concentration should I use?

There is no universal concentration. Build a ladder around the actual process range or a technically justified stress range and clearly define the concentration basis.

5. Is HASE always more electrolyte-tolerant than ASE?

No. HASE adds associative thickening, but salt response depends on hydrophobe architecture, pH, surfactants, binder and shear conditions.

6. Why can calcium or magnesium be more problematic than sodium?

Ca²⁺ and Mg²⁺ are divalent ions and can affect anionic polymers, dispersants and colloidal stability differently from monovalent sodium ions.

7. Should NaCl and CaCl2 be compared at the same weight percentage?

Not for a rigorous scientific comparison. They differ in molecular weight, ion valence and ionic strength. Factory tests should instead reproduce the actual process exposure or use a clearly defined comparison basis.

8. Why does the thickener pass the salt test but fail after binder is added?

Binder adds water, surfactants, electrolytes and polymer particles, and HASE-type thickeners can also interact associatively with the binder.

9. Should electrolyte tolerance be measured immediately or after holding?

Both. Immediate retention shows the first response, while holding-time retention reveals delayed instability that can matter during production.

10. Can I use electrolyte tolerance for incoming QC?

Yes, after the grade and method are validated. Use one standardized challenge and compare new batches with an approved reference, together with other agreed QC checks.

11. What is a good viscosity-retention percentage?

There is no universal percentage. The acceptance limit should come from successful production data and the minimum rheology needed for the actual printing process.

12. What should I send FSX Chemical for electrolyte-tolerance matching?

Send the current thickener/TDS, dosage, activation pH, viscosity method, pigment, binder, fixer, water hardness/conductivity, holding time and any current salt-test data.

Compare Synthetic Thickeners Under the Electrolyte Conditions That Matter

If a synthetic thickener builds strong viscosity in water but becomes unstable after pigment, binder, fixer or hard process water is added, FSX Chemical can help structure a controlled electrolyte-tolerance comparison.

একটি কার্যকর প্রযুক্তিগত পর্যালোচনার জন্য পাঠান:

  • আপনার বর্তমান সিন্থেটিক ঘনকারী নমুনা, TDS বা COA
  • Thickener dosage and activation method
  • চূড়ান্ত pH
  • সম্পূর্ণ সান্দ্রতা পরীক্ষা পদ্ধতি
  • Current salt-tolerance method if available
  • Pigment and binder products / dosages
  • Fixer / ionic auxiliaries
  • Water hardness / conductivity
  • Holding time
  • Current viscosity-retention or production-stability problem

দিয়ে শুরু করুন নমুনা ও মিলान নিয়ন্ত্রিত বর্তমান-বনাম-প্রার্থী মূল্যায়নের জন্য।.

পর্যালোচনা সিন্থেটিক প্রিন্টিং ঘনকারী বর্তমান FSX টেক্সটাইল-প্রিন্টিং থিকনার পরিসরের জন্য.

আপনিও করতে পারেন কারখানা-সরাসরি মূল্য উদ্ধৃতি অনুরোধ করুন after the suitable grade and electrolyte-tolerance working window are confirmed or এফএসএক্স কেমিক্যালের সাথে যোগাযোগ করুন প্রযুক্তিগত আলোচনা জন্য📧 ইমেইল: Service@fsxchemical.com

A meaningful electrolyte-tolerance number is never just “how much salt the thickener can take.” It is the viscosity and rheology retained under a clearly defined salt, concentration basis, pH, temperature, mixing and holding method—and finally the performance retained in the complete production paste.

দ্রুত লিঙ্কসমূহ

দ্রুত যোগাযোগ

আপনার প্রয়োজনীয়তা পাঠান

অথবা

বিনামূল্যে নমুনা · ২৪ ঘণ্টার প্রতিক্রিয়া

পণ্যের অনুসন্ধান ও সহায়তা

আপনার পণ্যের প্রয়োজনীয়তা পাঠান

পণ্যের নাম, ব্যবহার, পরিমাণ, গন্তব্য এবং আপনার কাছে থাকা যেকোনো TDS, নমুনা ছবি বা ডকুমেন্ট শেয়ার করুন। FSX Chemical এই তথ্য পর্যালোচনা করবে এবং কোটেশন, নমুনা মিলানো বা পণ্য নির্বাচনের পরবর্তী ধাপের জন্য পরামর্শ দেবে।.

পণ্যের তথ্য পণ্যের নাম, গ্রেড, মডেল, লেবেলের ছবি বা সরবরাহকারীর রেফারেন্স।.
উপলব্ধ নথিপত্র টিডিএস, এসডিএস, সিওএ, নমুনা ছবি, পণ্যের তালিকা বা পরীক্ষার তথ্য।.
অর্ডার বিবরণ আনুমানিক পরিমাণ, প্যাকেজিং, গন্তব্য দেশ, বন্দর বা বাণিজ্যিক শর্ত।.
আবেদন বা সমস্যা টেক্সটাইল প্রিন্টিং প্রক্রিয়া, ফর্মুলেশনের প্রয়োজন, বর্তমান সমস্যা বা লক্ষ্য কর্মক্ষমতা।.