Sodium Alginate for Hand Block Printing: Reactive Dye Paste, Trials and Troubleshooting

হ্যান্ড ব্লক প্রিন্টিংয়ের জন্য মেশিন স্ক্রিন প্রিন্টিংয়ের তুলনায় ভিন্ন প্রবাহগত বৈশিষ্ট্যের প্রিন্টিং পেষ্ট প্রয়োজন। এটি...
\n

Sodium alginate is a practical thickener for reactive-dye hand block printing on cellulosic fabrics when the paste requires clean transfer, controlled penetration and reliable wash-off. It should not be treated as a universal thickener for every traditional, natural-dye, mordant or resist process; suitability depends on the actual dye chemistry, alkali, salts, fabric and fixation route.

\n \n

This guide explains how to qualify textile-grade sodium alginate for hand block printing, including route screening, grade selection, small-batch preparation, workshop flow checks and production troubleshooting.

\n
\n

Is Sodium Alginate Suitable for This Hand-Printing Route?

\n\n\n
Process routeAlginate decisionMinimum trial
Reactive dye on cotton or viscoseStrong candidatePaste rheology, outline, fixation, wash-off
Pigment plus binderNot the default choiceBinder compatibility and handle
Natural dye or mordant routeDo not assume suitabilityExact recipe and full process sequence
Wax/resist plus printed reactive stageEvaluate only the color-paste stageBoundary control and post-wash result
\n\n\n

পেস্টের প্রয়োজনীয়তার দিক থেকে ব্লক প্রিন্টিং কীভাবে স্ক্রিন প্রিন্টিং থেকে পৃথক

ম্যানুয়াল প্রয়োগ এবং পেস্ট বডি

হাতে ব্লক প্রিন্টিং-এ খোদাই করা ব্লকটি প্রিন্টিং পেস্ট ভর্তি ট্রেতে চেপে দেওয়া হয় এবং তারপর হাতে কাপড়ে ছাপানো হয়। এই ম্যানুয়াল প্রয়োগ পদ্ধতির জন্য মেশিন স্ক্রিন প্রিন্টিং-এর তুলনায় ভিন্ন প্রবাহগত বৈশিষ্ট্যের পেস্ট প্রয়োজন।.

পেস্টটি এতটা ঘন হতে হবে যে তা ব্লকের মুখ সমানভাবে ঢেকে রাখতে পারে এবং ঝরে না পড়ে, পেস্ট ট্রে ও কাপড়ের মধ্যে ব্লকের পৃষ্ঠে তার আকৃতি ধরে রাখতে পারে, এবং ব্লক চাপিয়ে তুলে নেওয়ার সময় কাপড়ে পরিষ্কারভাবে ছেড়ে দিতে পারে। অতি তরল পেষ্ট ব্লক থেকে ঝরে পড়বে, অসমভাবে ছড়িয়ে পড়বে এবং কাপড়ে ছড়িয়ে যাবে। অতি ঘন পেষ্ট ব্লকে সমানভাবে লেপাবে না এবং নকশায় ফাঁক থাকতে পারে।.

\n

Block printing and rotary screen printing impose different transfer forces and dwell times. Set paste body from the actual block depth, tray or pad, fabric construction and required penetration; do not assume block printing always needs a higher viscosity.

\n

নকশার সংজ্ঞা এবং রঞ্জক স্থানচ্যুতি নিয়ন্ত্রণ

ব্লক প্রিন্টিং-এ নকশার সংজ্ঞা নির্ভর করে ছাপানোর পর পেষ্ট কাপড়ে রঞ্জককে ঠিক জায়গায় কতটা ভালোভাবে ধরে রাখে তার উপর। স্ক্রিন প্রিন্টিং-এর বিপরীতে, যেখানে যান্ত্রিক চাপের মাধ্যমে পেষ্টকে জালির মধ্য দিয়ে ঠেলে দেওয়া হয়, ব্লক প্রিন্টিং-এ পেষ্ট সরাসরি সংস্পর্শের মাধ্যমে স্থানান্তরিত হয়—ব্লকের পৃষ্ঠে থাকা পেষ্টের পাতলা স্তর চাপ পড়লে কাপড়ের পৃষ্ঠে চলে আসে।.

ট্রান্সফারের পর, পেষ্টের রঞ্জকটিকে স্থির না হওয়া পর্যন্ত সঠিক অবস্থানে থাকতে হবে। যদি পেষ্টের সান্দ্রতা অপর্যাপ্ত হয়, কাপড়ের ক্যাপিলারি ক্রিয়া ছাপানো এলাকা থেকে রঞ্জককে বাইরের দিকে টেনে নিয়ে যায়, ফলে প্যাটার্নের প্রান্তে ব্লিডিং সৃষ্টি হয়। সোডিয়াম অ্যালজিনেটের ছদ্মপ্লাস্টিক আচরণ—বিশ্রামে উচ্চ সান্দ্রতা, চাপ প্রয়োগে নিম্ন সান্দ্রতা—ব্লক প্রিন্টিংয়ের জন্য অত্যন্ত উপযোগী, কারণ ব্লক চাপলে পেষ্ট সহজে প্রবাহিত হয়, কিন্তু চাপ সরিয়ে নিলে তা নির্দিষ্ট স্থানে স্থির থাকে।.

ব্যাচের আকার এবং প্রস্তুতির স্কেল

ব্লক প্রিন্টিং কার্যক্রম—প্রথাগত কারিগর কর্মশালা হোক বা ছোট বাণিজ্যিক উদ্যোগ—সাধারণত শিল্পায়িত স্ক্রিন প্রিন্টিংয়ের তুলনায় ছোট ব্যাচে পেষ্ট প্রস্তুত করে। প্রতি রঙের পেষ্টের পরিমাণ প্রায়ই শত শত লিটারের পরিবর্তে লিটারে পরিমাপ করা হয়, এবং পেষ্ট প্রস্তুতি হাতে বা ছোট আকারের মিক্সিং যন্ত্রপাতি দিয়ে করা হয়।.

\n

Small batches make preparation variables more visible. Add powder gradually to controlled-temperature water under adequate agitation, allow full hydration, then filter and rest the paste according to the approved method. Mesh size can affect wetting and dispersion, but it does not by itself predict hydration speed, viscosity or print quality.

\n

প্রতিক্রিয়াশীল রঞ্জক ব্লক প্রিন্টিং পেস্টে সোডিয়াম অ্যালজিনেট

\n

Typical Components to Validate in a Reactive-Dye Block Paste

\n

একটি রিঅ্যাক্টিভ ডাই ব্লক প্রিন্টিং পেষ্টে স্ক্রিন প্রিন্টিং পেষ্টের মূল উপাদানগুলোই থাকে — সোডিয়াম অ্যালজিনেট, রিঅ্যাক্টিভ ডাই, ক্ষার, ইউরিয়া এবং অ্যান্টি-রিডাক্টিং এজেন্ট — তবে ব্লক প্রয়োগের জন্য সাধারণত প্রয়োজনীয় উচ্চ সান্দ্রতা অর্জনের জন্য এদের অনুপাত ভিন্ন হতে পারে।.

ব্লক প্রিন্টিং পেষ্টে সোডিয়াম অ্যালজিনেটের ঘনত্ব প্রায়ই স্ক্রিন প্রিন্টিং-এ ব্যবহৃত পরিসরের উচ্চ প্রান্তের দিকে থাকে, অথবা একই ঘনত্বে উচ্চ সান্দ্রতা গ্রেড ব্যবহার করা হয়, যাতে পেষ্টের গঠন ব্লক কোটিং করার সময় ঝরে না পড়ে পর্যাপ্ত হয়। নির্দিষ্ট ঘনত্ব নির্ভর করে সান্দ্রতা গ্রেড, কর্মশালার পরিবেশগত তাপমাত্রা এবং ব্লকে প্রিন্টারের পেস্টের আচরণ সম্পর্কে তার মূল্যায়নের উপর।.

প্রচলিত কারিগরি পরিবেশে, পেস্টের ফর্মুলেশন প্রায়শই অভিজ্ঞতাভিত্তিকভাবে তৈরি করা হয় — ভিসকোমিটার পরিমাপের পরিবর্তে প্রিন্টার দৃশ্যগত ও স্পর্শগত মূল্যায়নের ভিত্তিতে পেস্টের আচরণ সামঞ্জস্য করে। অভিজ্ঞতাভিত্তিক থেকে পরিমাপভিত্তিক ফর্মুলেশনে রূপান্তরিত হওয়া অপারেশনের জন্য, পরিমাপের মাধ্যমে একটি লক্ষ্যমাত্রা সান্দ্রতা পরিসীমা নির্ধারণ করা এবং তা পরিচিত ভালো পেস্ট আচরণের সাথে সম্পর্কিত করা একটি কার্যকর প্রথম ধাপ।.

ছোট ব্যাচের ব্লক প্রিন্টিং-এ ক্ষার ব্যবস্থাপনা

শিল্পক্ষেত্রে স্ক্রিন প্রিন্টিং-এ ক্ষারযুক্ত পেস্ট বড় পরিমাণে প্রস্তুত করা হয় এবং নির্দিষ্ট সময়সীমার মধ্যে ব্যবহার করা হয়। ছোট ব্যাচের ব্লক প্রিন্টিং-এ একই নীতি প্রযোজ্য, তবে বাস্তবিক কিছু ভিন্ন সীমাবদ্ধতা রয়েছে — ছোট ব্যাচগুলো দিনজুড়ে বিচ্ছিন্নভাবে প্রস্তুত ও ব্যবহার করা যেতে পারে, এবং প্রিন্টিং সেশনের মধ্যে পেস্ট ট্রেতে রেখে দেওয়া যেতে পারে।.

পেস্টটিতে একবার ক্ষার যোগ করলে সোডিয়াম অ্যালজিনেটের ক্ষার-উদ্দীপিত অবক্ষয় অবিরামভাবে চলে, এবং তাপমাত্রা বাড়ার সাথে সাথে এর হার বৃদ্ধি পায়। উষ্ণ কর্মশালা পরিবেশে, ক্ষার যোগের পর কয়েক ঘণ্টার মধ্যে পেস্টের সান্দ্রতা লক্ষণীয়ভাবে কমে যেতে পারে। ব্যবহারিক বিকল্পগুলো হলো:

  • ক্ষারবিহীন পেস্ট প্রস্তুত করুন এবং মুদ্রণ সেশনের ঠিক আগে ক্ষার যোগ করুন, সেশনের শেষে অব্যবহৃত ক্ষারযুক্ত পেস্ট ফেলে দিন।
  • ক্ষার হিসেবে সোডিয়াম কার্বনেটের পরিবর্তে সোডিয়াম বাইকার্বনেট ব্যবহার করুন — বাইকার্বনেট ধীরে ধীরে ক্ষারত্ব প্রদান করে এবং কার্বনেটের তুলনায় পেস্টের ব্যবহারযোগ্য সময় বাড়ায়।
  • প্রিন্টিং সেশনগুলোর মধ্যে পেস্টকে অবক্ষয় ধীর করতে ঠান্ডা পরিবেশে রাখুন।

যদি প্রিন্টিং সেশনের সময় পেস্টের সান্দ্রতা লক্ষণীয়ভাবে কমে যায় এবং প্রিন্টের গুণমান খারাপ হয়ে যায়, তাপমাত্রা স্থির থাকলে এবং অন্য কোনো পরিবর্তন না হলে অ্যালকালি অবক্ষয়ই সবচেয়ে সম্ভাব্য কারণ।.

প্রাকৃতিক রঞ্জক ঐতিহ্য এবং সোডিয়াম অ্যালজিনেট সামঞ্জস্য

\n

Natural-dye, mordant and resist traditions use many process routes. Before introducing sodium alginate, run a small compatibility trial with the exact colorant, mordant, alkali, water quality, fabric and fixation sequence. Evaluate shade, outline, penetration and wash-off rather than assuming transfer from a reactive-dye recipe.

\n \n

Where a mordant or auxiliary is part of the paste, add it only after confirming compatibility and holding stability. Compare a fresh paste with the intended workshop holding time and check for viscosity drift, separation or loss of print definition.

\n \n

Control pH using the dye supplier’s process window. Sodium alginate tolerates many reactive-printing conditions, but the complete paste—not the thickener alone—must be tested after alkali and electrolyte addition.

\n

আজরাখ প্রিন্টিং: প্রক্রিয়া এবং আঠার প্রয়োজনীয়তা

\n

Ajrak is a multistage resist, mordant and dyeing tradition with workshop-specific recipes. The process should be documented before recommending any thickener; sodium alginate is relevant only when a compatible printed color or reactive-dye stage is actually used.

\n \n

If a workshop uses a reactive-dye paste on cotton within an Ajrak-inspired or mixed production route, sodium alginate can be screened for outline control and wash-off. This is an application-specific trial, not a general prescription for traditional Ajrak.

\n \n

For multistage work, test the alginate paste through the complete sequence—including drying, steaming or curing, washing and any later resist or mordant steps—to detect interactions that a single stamp test will miss.

\n

বাগরু ও সাঙ্গানার ব্লক প্রিন্টিং (ভারত)

\n

Bagru and Sanganer workshops use diverse natural, pigment and reactive color systems. Identify the actual route first. For reactive-dye printing on cellulosic fabric, sodium alginate may be evaluated; other systems need a thickener selected for their own binder, mordant and fixation chemistry.

\n \n

Do not select a “medium-viscosity” grade by label alone. Compare samples at equal solids and a defined test method, then adjust concentration to the block depth, fabric absorbency and desired penetration. Approve the grade only after print, fixation and wash-off trials.

\n

ব্যাটিক এবং মোম প্রতিরোধী ছাপাই

\n

In batik and other resist processes, the wax or resist stage and the color-application stage should be evaluated separately. Sodium alginate may be considered only for a compatible reactive-dye printing stage.

\n \n

Where an alginate paste is used alongside a resist, choose rheology from trial results: the paste must transfer without flooding fine resist boundaries, while still wetting the exposed fabric. A universal low-, medium- or high-viscosity recommendation is not reliable.

\n

শিল্পী ও ক্ষুদ্র-পরিসরের ব্লক প্রিন্টিংয়ের জন্য গ্রেড নির্বাচন

সান্দ্রতা গ্রেড বিবেচ্য বিষয়সমূহ

হাতে ব্লক প্রিন্টিং পেস্টের জন্য সাধারণত মাঝারি থেকে উচ্চ সান্দ্রতার সোডিয়াম অ্যালজিনেট গ্রেডগুলো সবচেয়ে উপযুক্ত। ম্যানুয়াল ব্লক প্রয়োগ পদ্ধতিতে এমন পেস্টের প্রয়োজন যা ব্লকের পৃষ্ঠে ঝরে না পড়ে ধরে থাকে — একটি বৈশিষ্ট্য যা নিম্ন সান্দ্রতার গ্রেডগুলো প্রচলিত ব্যবহার ঘনত্বে প্রদান করে না।.

যদি আপনি পরীক্ষামূলকভাবে তৈরি পেস্ট থেকে নির্দিষ্ট সোডিয়াম অ্যালজিনেট গ্রেডে পরিবর্তন করছেন, তাহলে প্রথমে নির্ধারিত তাপমাত্রায় আপনার বিদ্যমান পেস্টের সান্দ্রতা পরিমাপ করে সেটিকে নতুন গ্রেডের লক্ষ্য হিসেবে ব্যবহার করুন। এটি গ্রেডের স্পেসিফিকেশনকে আপনার পরিচিত কার্যকরী পেস্ট আচরণের সাথে সংযুক্ত করে।.

ক্ষুদ্র-পরিসরের প্রস্তুতিতে দ্রবণীকরণ পদ্ধতি

শিল্পী-নির্মিত ছোট ব্যাচের প্রস্তুতিতে ঠান্ডা পানিতে দ্রবীভূত করা ব্যবহারিক এবং তাপীয় যন্ত্রপাতির প্রয়োজনীয়তা এড়ায়। মূল বিষয় হল পাউডারটি ক্রমাগত নাড়তে নাড়তে ধীরে ধীরে পানিতে যোগ করা—কম পরিমাণের জন্য কাঠ বা প্লাস্টিকের প্যাডেলই যথেষ্ট—এবং ব্যবহারের আগে সম্পূর্ণ হাইড্রেশন নিশ্চিত করতে পর্যাপ্ত সময় দেওয়া।.

সূক্ষ্ম জাল গ্রেড (৬০ জাল এবং তার বেশি) হালকা হাতে মিশানোর শর্তে মোটা জাল গ্রেডের তুলনায় সহজে দ্রবীভূত হয়। যেখানে মিশানোর যন্ত্রপাতি সাধারণ এবং মিশানোর সময় সীমিত, সেই কারুশিল্প প্রক্রিয়ায় সূক্ষ্ম জাল গ্রেড পেস্টে অপর্যাপ্ত দ্রবণ ও গুটি বাঁধার ঝুঁকি কমায়।.

পরিচ্ছন্ন প্যাটার্ন সংজ্ঞার জন্য বিশুদ্ধতা ও দ্রাব্যতা

\n

For procurement, specify the supplier’s test method and acceptance range for viscosity, moisture, pH and insoluble matter. Compare certificate results with an incoming-lot hydration and filtration check; do not rely on one generic insoluble-matter limit across all grades.

\n

প্রিন্ট করা ফ্যাব্রিক যদি ক্রেতার বস্ত্র রাসায়নিকগুলিতে ভারী ধাতুর পরিমাণ সংক্রান্ত নির্দিষ্টকরণের আওতায় পড়ে—যা প্রধান খুচরা বাজারের রপ্তানি অর্ডারে ক্রমশ সাধারণ—তাহলে সোডিয়াম অ্যালগিনেটে থাকা ভারী ধাতুর পরিমাণ প্রাসঙ্গিক হতে পারে। যদি আপনার চূড়ান্ত বাজারে এটি প্রয়োজন হয়, তবে আপনার সরবরাহকারীর কাছ থেকে ভারী ধাতুর তথ্য অনুরোধ করুন।.

ব্লক প্রিন্টিংয়ের জন্য ব্যবহারিক পেস্ট মূল্যায়ন

\n

Workshop Flow Checks (Not a Substitute for Viscosity Testing)

\n \n

When a viscometer is unavailable, use drip, block-face and stamp checks to compare a new batch against an approved reference paste. Record water temperature, mixing time, rest time and concentration so the comparison is repeatable.

\n
  • ড্রিপ পরীক্ষা — পেস্ট থেকে একটি প্যাডেল তুলে দেখুন পেস্টটি অবিরত পড়ছে নাকি সামান্য ধরে রেখে তারপর পড়ছে; ব্লক প্রিন্টিংয়ের জন্য পর্যাপ্ত ঘনত্বের পেস্ট প্রথম ফোঁটা পড়ার আগে ২–৩ সেকেন্ড ধরে রাখতে হবে।
  • ব্লক ফেস টেস্ট — ব্লকটি পেস্ট ট্রে-তে চাপুন এবং তুলে নিন; ব্লকের পৃষ্ঠে পেস্টটি খোদাই করা নকশার সর্বনিম্ন বিন্দু থেকে ফোঁটা ছাড়াই সমানভাবে লেপিত হওয়া উচিত।
  • স্ট্যাম্প পরীক্ষা — পেস্ট-ভরা ব্লকটি আপনার উৎপাদন ফ্যাব্রিকের নমুনায় ছাপিয়ে দেখুন এবং মূল্যায়ন করুন প্যাটার্নের প্রান্তগুলো তীক্ষ্ণ আছে নাকি ছড়িয়ে পড়ছে।
\n

These workshop checks show transfer behavior but do not produce a procurement-grade viscosity value. Supplier and incoming QC comparisons should use the same instrument, spindle, speed, temperature, solution concentration and hydration time.

\n

সামঞ্জস্যতার জন্য একটি রেফারেন্স পেস্ট স্থাপন

যে সব প্রক্রিয়ায় অনুমানভিত্তিকভাবে পেষ্ট তৈরি করা হয়, সেক্ষেত্রে পরিমাপকৃত ঘনত্ব, পরিমাপকৃত সান্দ্রতা, নথিভুক্ত সোডিয়াম অ্যালজিনেট গ্রেড ও লট নম্বরসহ নিশ্চিত কার্যকরী পরামিতিতে একটি রেফারেন্স ব্যাচ প্রস্তুত করে তা মানগত রেফারেন্স হিসেবে সংরক্ষণ করলে ভবিষ্যতের ব্যাচগুলোর তুলনার জন্য একটি পুনরাবৃত্তিমূলক মানদণ্ড পাওয়া যায়। সোডিয়াম অ্যালজিনেটের লট বা সরবরাহকারী পরিবর্তন করার সময় এটি বিশেষভাবে কার্যকর, কারণ রেফারেন্স ব্যাচের সঙ্গে সরাসরি পাশাপাশি তুলনা উৎপাদন প্রভাবিত হওয়ার আগেই কর্মক্ষমতার যেকোনো পার্থক্য চিহ্নিত করে।.

\n

প্রায়শই জিজ্ঞাসিত প্রশ্নাবলী

\n\n\n
Is sodium alginate suitable for every hand block printing process?\n

No. It is primarily evaluated for compatible reactive-dye pastes on cellulosic fabric. Natural-dye, pigment, mordant and resist systems require separate compatibility trials.

\n
\n\n\n
How should a workshop choose sodium alginate viscosity?\n

Compare candidate grades at controlled solids, then adjust concentration against block depth, fabric absorbency, outline and penetration. Confirm the value using a documented viscosity method.

\n
\n\n\n
Can a drip test replace a viscometer?\n

No. A drip or stamp test is useful for daily comparison with an approved paste, but supplier qualification and incoming QC require method-controlled viscosity measurement.

\n
\n\n\n
When should alkali be added to a reactive block-printing paste?\n

Follow the dye-system procedure and add alkali as late as practical when limited paste stability is a concern. Validate the intended holding time under actual workshop temperature.

\n
\n\n\n
What should be recorded during a sample trial?\n

Record grade and lot, solids, water temperature, mixing and rest time, additives, fabric, block geometry, fixation, wash-off, outline and final shade. For a supplier comparison, use নমুনা ও মিলान.

\n
\n\n\n\n

FSX কেমিক্যাল কীভাবে শিল্পী ও ক্ষুদ্র-পরিসরের মুদ্রণ কার্যক্রমকে সমর্থন করে

FSX কেমিক্যাল হ্যান্ড ব্লক প্রিন্টিং, কারিগরি রিঅ্যাক্টিভ ডাই প্রয়োগ এবং ছোট পরিসরের স্ক্রিন প্রিন্টিং অপারেশনের জন্য উপযোগী সোডিয়াম অ্যালজিনেটের গ্রেড সরবরাহ করে। স্ট্যান্ডার্ড বাল্ক অর্ডারের ন্যূনতম পরিমাণের নিচে নমুনা পরিমাণ মূল্যায়নের জন্য পাওয়া যায়, যা বিশেষ করে কারিগরি অপারেশনগুলোর জন্য প্রাসঙ্গিক, যারা বড় পরিমাণে ক্রয়ের আগে একটি গ্রেড পরীক্ষা করতে চায়।.

প্রতিটি গ্রেডের জন্য সান্দ্রতা, মেশ স্পেসিফিকেশন, ডিএস এবং দ্রবণ নির্দেশিকা অন্তর্ভুক্ত করে টেকনিক্যাল ডেটাশীটসমূহ উপলব্ধ। যদি আপনি কোনো নির্দিষ্ট ব্লক প্রিন্টিং ঐতিহ্যের জন্য পেস্ট ফর্মুলেশন তৈরি করছেন বা ছোট পরিসরের উৎপাদনে পেস্ট সংক্রান্ত সমস্যা সমাধান করছেন, তাহলে আমাদের টেকনিক্যাল টিম গ্রেড নির্বাচন ও ফর্মুলেশন নির্দেশিকায় সহায়তা করতে পারে।.

পরবর্তী পদক্ষেপ:

দ্রুত যোগাযোগ

আপনার প্রয়োজনীয়তা পাঠান

অথবা

বিনামূল্যে নমুনা · ২৪ ঘণ্টার প্রতিক্রিয়া

পণ্যের অনুসন্ধান ও সহায়তা

আপনার পণ্যের প্রয়োজনীয়তা পাঠান

পণ্যের নাম, ব্যবহার, পরিমাণ, গন্তব্য এবং আপনার কাছে থাকা যেকোনো TDS, নমুনা ছবি বা ডকুমেন্ট শেয়ার করুন। FSX Chemical এই তথ্য পর্যালোচনা করবে এবং কোটেশন, নমুনা মিলানো বা পণ্য নির্বাচনের পরবর্তী ধাপের জন্য পরামর্শ দেবে।.

পণ্যের তথ্য পণ্যের নাম, গ্রেড, মডেল, লেবেলের ছবি বা সরবরাহকারীর রেফারেন্স।.
উপলব্ধ নথিপত্র টিডিএস, এসডিএস, সিওএ, নমুনা ছবি, পণ্যের তালিকা বা পরীক্ষার তথ্য।.
অর্ডার বিবরণ আনুমানিক পরিমাণ, প্যাকেজিং, গন্তব্য দেশ, বন্দর বা বাণিজ্যিক শর্ত।.
আবেদন বা সমস্যা টেক্সটাইল প্রিন্টিং প্রক্রিয়া, ফর্মুলেশনের প্রয়োজন, বর্তমান সমস্যা বা লক্ষ্য কর্মক্ষমতা।.